Category 类 别 | Trade- Mark 牌 号 | Equivalent to China Standard 相当国标 | Characteristics & application 特性和用途 | Equivalent to AWS 相当AWS |
Hard-surfacing 硬 面 堆 焊 | D 667 | EDZCr-B-15 | HRc≥48. Resistance to wear, gas corrosion and oxidation. Hardfacing of blast furnace hopper and cracker part. HRc≥48,耐磨、耐气蚀、抗氧化。堆焊高炉料钟、破碎机件 | |
D 802 | EDCoCr-A-03 | HRc38-47. Resistance to heat, wear and corrosion. Hardfacing of high temperature part such as the edge of thermo-cutter. HRc38-47,耐热、耐蚀、耐磨。堆焊高温工件如热剪切刀刃 | ECoCr-A | |
D 812 | EDCoCr-B-03 | HRc45-50. Resistance to heat, wear and corrosion. Hardfacing of high temperature part such as internal-combustion engine valve. HRc45-50,耐热、耐蚀、耐磨。堆焊高温工件如内燃机阀 | ECoCr-B | |
D 822 | | HRc≥53. Resistance to Wear and heat, bad shock resistance. Hardfacing of rotating blade wheel of boiler. HRc≥53,耐热、耐磨,但抗冲击性差。堆焊锅炉旋转叶轮 | | |
D 832 | EDCoCr-C-03 | HRc≥50. Wear and heat resistance. Hardfacing of high temperature part such as hot-rolling guided way. HRc≥50,耐热、耐磨。堆焊高温工件如热轧导轨 | ECoCr-C | |
D 842 | EDCoCr-D-03 | HRc28-38. Corrosion and thermo-fatigue resistance, work harding. Hardfacing of hot forging die. HRc28-38,耐蚀、抗热疲劳,具有加工硬化性。堆焊热锻模 | | |
Cast iron 铸 铁 | Z 308 | EZNi | Pure nickel, excellent general properties. Used to weld thin cast iron part and repair welding machined surface, such as guided way of machine tool. 纯镍,综合性能好。铸铁薄件及加工面补焊用,如机床导卫 | ENi-Cl |
Z 408 | EZNiFe | Iron nickel, high strength and excellent ductility. Repair welding of important gray cast iron and nodular cast iron, such as cylinder cap. 镍铁,强度高、塑性好。重要灰铸铁及球铁焊补用,如汽缸盖 | ENiFe-Cl | |
Z 508 | EZNiCu-1 | Copper nickel, good machinability and bad crack resistance. Repair welding of sand hole and gray cast iron machined surface subject to no load. 镍铜,易加工,但抗裂性较差。不受力的灰铸铁加工面及砂眼补焊 | ENiCu-B | |
Copper alloys 铜 合 金 | Cu 107 | ECu | Red copper, atmosphere and sea water corrosion and excellent electric conductivity. Welding of red copper such as electrical copper row. 紫铜,耐大气,海水腐蚀,导电性好。紫铜焊接用,如导电铜排 | ECu |
Cu 207 | ECuSi | Silicon bronze, corrosion resistance and high strength. Welding of copper, silicon bronze and brass. 硅青铜,耐蚀、强度高。铜、硅青铜及黄铜焊接用 | ECuSi | |
Cu 227 | ECuSnB | Tin phosphor bronze, corrosion resistance and high strength. Welding of copper, silicon bronze and brass. 锡磷青铜,耐蚀、强度高。铜、硅青铜及黄铜焊接用 | ECuSn-C | |
Cu 237 | ECuAl | Aluminum bronze, wear and corrosion and high strength. Welding or surfacing of copper alloys. 铝青铜,耐磨、耐蚀,强度高。铜合金焊接或堆焊用 | ECuAl-A2 | |
Aluminum alloys 铝 合 金 | Al 109 | TAl | Pure aluminum, excellent corrosion resistance and middle strength. Welding of pure aluminum. 纯铝,耐蚀性好,但强度不高,纯铝焊接用 | E1100 |
Al 209 | TAlSi | Silicon aluminum, good crack resistance and wide range of usage. Welding of aluminum alloys other than aluminum magnesium alloys. 铝硅,抗裂性好,通用性大。铝合金焊接用,不宜焊接铝镁合金 | E4043 | |
Al 309 | TAMn | Manganese aluminum, corrosion resistance and high strength. Welding of aluminum alloys. 铝锰,强度高,耐蚀。铝合金焊接用 | E3003 | |
Nickel alloys 镍合金 | Ni 102 | ENi-1 | Pure nickel. Welding and surfacing of nickel and nickel to steel. 纯镍,用于镍、镍与钢的焊接与堆焊 | ENi-1 |
Ni 207 | ENiCu-7 | Copper nickel. Welding and surfacing of copper nickel and copper nickel to steel. 镍铜,用于镍铜、镍铜与钢的焊接与堆焊 | ENiCu-7 |
Category 类 别 | Trade mark 牌 号 | Chemical composition 主要成份(%) | Characteristics & application 特性和用途 | Equivalent to AWS 相当AWS |
Hardfacing 硬 面 堆 焊 | S 101 | C3 Cr28 Ni4 Si3.5 Fe Rem. | HRc48-54. Resistance to wear, gas corrosion and oxidation. Hardfacing of bucket tooth and case pump. HRc48-54,耐磨、耐气蚀、抗氧化。堆焊铲斗齿,泵套 | |
S 111 | C1 Cr29 W5 Co Rem. | HRc38-47. Resistance to wear and corrosion at high-temperature. Hardfacing of high temperature and pressure valve. HRc38-47,高温下耐磨、耐蚀。堆焊高温高压阀门 | ECoCr-A | |
S 112 | C1.5 Cr29 W8 Co Rem. | HRc45-50. Resistance to wear and corrosion at high-temperature. Hardfacing of valve and hot-rolling pass. HRc45-50,高温下耐磨、耐蚀。堆焊阀门,热轧孔型 | ECoCr-B | |
S 113 | C2.5 Cr30 W17 Co Rem. | HRc≥55. Wear and heat resistance at high temperature, bad shock resistance. Hardfacing of screw charging carriage. HRc≥55,高温下耐磨、耐热,但抗冲击性差。堆焊螺旋送料机用 | | |
S 114 | C2.5 Cr30 W12 Co Rem. | HRc≥53. Wear and heat resistance at high temperature, bad shock resistance. Hardfacing of three-cone bit. HRc≥53,高温下耐磨、耐热,但抗冲击较差。堆焊牙轮钻头 | ECoCr-C | |
Copper alloys 铜 合 金 | S 201 | Sn1 Si0.3Mn0.3 Cu Rem. | Good mechanical properties and crack resistance. Gas welding and argon arc welding of red copper. 机械性能好,抗裂性好。紫铜气焊及氩弧焊用 | ERCu |
S 211 | Si3 Mn1 Cu Rem. | Good mechanical properties. Argon arc welding of copper alloys and MIG brazing of steel. 机械性能好,铜合金氩弧焊及钢的MIG钎焊用 | ERCuSi-Al | |
S 212 | Sn5 Cu Rem. | Wear resistance. Argon arc welding of copper alloys and surfacing of steel. 耐磨性好。铜合金氩弧焊及钢的堆焊用 | ERCuSn-A | |
S 213 | Sn8 Cu Rem. | Wear resistance. Argon arc welding of copper alloys and surfacing of steel. 耐磨性好。铜合金氩弧焊及钢的堆焊用 | ERCuSn-C | |
S 214 | Al7.5 Cu Rem. | Wear and corrosion resistance. Argon arc welding of copper alloys and surfacing of steel. 耐磨、耐蚀。铜合金氩弧焊及钢的堆焊用 | ERCuAl-A1 | |
S 215 | Al9 Cu Rem. | Wear and corrosion resistance. Argon arc welding of copper alloys and surfacing of steel. 耐磨、耐蚀。铜合金氩弧焊及钢的堆焊用 | ERCuAl-A2 | |
S 221 | Cu60 Sn1 Si0.3 Zn Rem. | Melting point is about 890℃. Gas welding and carbon arc welding of brass, also braze welding of copper, steel and cast iron. 熔点约890℃。黄铜气焊及碳弧焊用,也可钎焊铜、钢、铸铁 | | |
S 221F | Cu60 Sn1 Si 0.3 Zn Rem. | S221 welding rod coated with flux. 外涂焊剂的S221焊丝 | | |
S 222 | Cu58Sn0.9Si0.1 Fe0.8 Zn Rem. | Melting point is about 880℃. Gas welding and carbon arc welding of brass, also braze welding of copper, steel and cast iron. 熔点约880℃。黄铜气焊及碳弧焊用,也可钎焊铜、钢、铸铁 | RBCuZn-C | |
S 222F | Cu58Sn0.9Si0.1 Fe0.8 Zn Rem. | S222 welding rod coated with flux. 外涂焊剂的S222焊丝 | RBCuZn-C | |
S 223 | Cu59 Sn0.6 Zn Rem. | Melting point is about 900℃. Braze welding of copper, steel and cast iron. 熔点约900℃。铜、钢、铸铁钎焊用 | RBCuZn-A | |
S 224 | Cu62 Si0.5 Zn Rem. | Melting point is about 905℃. Gas welding and carbon arc welding of brass, also braze welding of copper, steel and cast iron. 熔点约905℃。黄铜气焊及碳弧焊用,也可钎焊铜、钢、铸铁 | | |
Copper alloys 铜 合 金 | S 225 | Cu48 Ni10 Zn Rem. | Melting point is about 935℃ and high strength. Braze welding of steel, nickel and carbide alloys. 熔点约935℃。高强度,钎焊钢、镍及硬质合金用 | RBCuZn-D |
S 225F | Cu48 Ni10 Zn Rem. | S225 welding rod coated with flux. 外涂焊剂的S225焊丝 | RBCuZn-D | |
S 226 | Cu60 Sn0.3 Si0.2 Zn Rem. | Melting point is about 900℃. Gas welding of brass, also braze welding of copper, steel and cast iron. 熔点约900℃。黄铜气焊用,也可钎焊铜、钢、铸铁 | | |
S 227 | Cu58Sn0.9Ni0.5 Si0.1 Fe0.8 Zn Rem. | Melting point is about 880℃. Gas welding and carbon arc welding of brass, also braze welding of copper, steel and cast iron. 熔点880℃。黄铜气焊及碳弧焊用,也可钎焊铜、钢、铸铁 | RBCuZn-B | |
S 229 | Cu55 Ni6 Mn4 Zn余 | Melting point is about 920℃, high strength. Braze welding of steel, nickel and hard carbide. 熔点约920℃。高强度,钎焊钢、镍及硬质合金用 | | |
Aluminum alloys 铝 合 金 | S 301 | Al≥99.5 | Good ductility and corrosion resistance. Gas welding and argon arc welding of pure aluminum. 塑性好、耐蚀。纯铝气焊、氩弧焊用 | ER1100 |
S 311 | Si5 Al Rem. | Corrosion resistance, wide range of usage. Gas welding and argon arc welding of aluminum alloys other than high magnesium alloys. 抗裂性好,通用性大。铝合金气焊、氩弧焊用。不宜用高镁合金 | ER4043 | |
S 321 | Mn1.3 Al Rem. | Good corrosion resistance, weldability and ductility. Gas welding and argon arc welding of aluminum alloys. 良好的耐蚀性、可焊性及塑性。铝合金气焊、氩弧焊用 | | |
S 331 | Mg5 Mn0.4 Al Rem. | Corrosion resistance and high strength. Argon arc welding of aluminum alloys. 耐蚀,强度高。铝合金氩弧焊用 | ER5183 |